Shot peening explained

Intensity, coverage, Almen strips and the controls that make peening repeatable.

By Surface Technologies engineering · Updated November 27, 2026 · 2 min read

What peening does

Each impact plastically deforms the surface and leaves a residual compressive stress beneath it. Cracks start in tension, so a compressed surface layer resists fatigue, stress corrosion and fretting.

Intensity

Measured with Almen strips: a standard steel strip is peened, released and its arc height read. The intensity spec (for example 0.008 to 0.012 A) sets media, velocity and angle.

Coverage

The percentage of the surface dented at least once. Specs call for 100% or more (200% means twice the time it took to reach 100%).

Controls that matter

Wheel or nozzle speed, media flow rate, part rotation, cycle time and media condition all need to be set and logged. Controls that record each run against a recipe let an auditor trace it.

Where it's used

Gears, shafts, springs, connecting rods, turbine blades, landing gear and fasteners. AMS 2430 and AMS 2432 are the common specifications.

The specifications you will meet

SAE AMS 2430 covers automatic shot peening and AMS 2432 adds computer-monitored control for critical parts. SAE J443 describes the use of Almen strips and J442 the strips and gauge themselves. Automotive and aerospace OEMs add their own process specifications on top, and the drawing callout is what governs.

Building a saturation curve

To set up a job, strips are peened for increasing exposure times and their arc heights plotted. Intensity is defined at the point where doubling the exposure raises the arc height by no more than ten percent. Running at or beyond that point means small variations in time do not change the result.

Media condition

Broken shot has sharp edges that can nick the surface and start the cracks peening is meant to prevent. Peening machines therefore classify media continuously by size and, on critical work, by shape, removing fragments and undersize particles. Media checks are part of the process record.

Masking and fixturing

Areas that must not be peened, such as threads, bearing journals and sealing faces, are masked with tape, plugs or purpose-made tooling. Fixtures hold the part so the stream reaches fillets and roots at the specified angle. On repeat work the fixture is as much part of the process as the nozzle.

Peening versus other treatments

Peening is often compared with case hardening, nitriding and roller burnishing. It is complementary to heat treatment rather than a substitute: carburised gears are peened after hardening to add compressive stress at the root. Its advantages are that it works on finished geometry, at room temperature, with little dimensional change.